Magnesium is one of the few structural metals the body can absorb. Under the right conditions an implanted magnesium part corrodes, and the body takes up and clears what it releases. That is less surprising than it sounds: magnesium is an essential mineral, and many people take it as a supplement. Its stiffness is also far closer to that of cortical bone than titanium’s is.
Most bone fixation today uses titanium plates and screws. Once the bone has healed, that hardware either comes out in a second surgery or stays in the body for life.
Lupine Research is among the companies and research groups working to make magnesium fixation hardware practical. The idea is simple: the magnesium holds the bone for as long as healing takes, and is then absorbed.
The difficulty is speed. Bare magnesium corrodes too quickly in body fluid. The part can lose its strength before the bone has healed, and the reaction releases hydrogen gas that the surrounding tissue has to clear. The corrosion has to be slowed.
Plasma electrolytic oxidation (PEO), also called micro-arc oxidation (MAO), is the most widely used way to do that. But “PEO coated” covers a wide range. Coatings of the same thickness, on the same alloy, can give very different protection. This note explains where the protection comes from and shows how we measure it, with data from our own coatings. The same reasoning applies to magnesium parts outside the body, wherever salt water is the problem.
Two layers, and one of them does the work
A PEO coating is not deposited onto the part. It is grown from the part: the magnesium is immersed in a dilute alkaline electrolyte and driven to several hundred volts, and thousands of short-lived micro-discharges convert the surface into a ceramic oxide.

Those discharges leave a characteristic structure with two layers.
- A porous outer layer makes up most of the thickness. Every discharge leaves a channel as it solidifies, so this layer is full of pores and fine cracks, many of them open to the surface.
- A dense inner barrier layer sits against the metal. It is thin, typically a micron or less, and it provides most of the corrosion resistance.
The practical consequence is that thickness is a poor measure of protection. Chloride solution moves quickly through the outer layer’s open pores. What holds it back is the barrier layer, and the ways of making a coating thicker (more time, more current) also produce larger, more energetic discharges that can damage that barrier.
What controls the result
Four things decide how protective a PEO coating on magnesium turns out to be.
| Lever | What it changes | Trade-off |
|---|---|---|
| Electrolyte chemistry | Which phases form. Phosphate baths give magnesium oxide with magnesium phosphate; silicate baths give harder forsterite; fluoride additions give dense, stable magnesium fluoride; calcium-bearing baths add calcium phosphate for implant surfaces. | Every bath element ends up in the coating, which matters for implants and for downstream processing. |
| Electrical regime | The size and number of discharges. Pulsed power, and bipolar pulsing in particular, is generally reported to give denser coatings than plain DC. | The best waveform depends on the alloy and the bath. Settings do not transfer between them unchanged. |
| Alloy and surface preparation | How uniformly the coating starts. Second phases, machining damage, and mill scale all show up as weak points. | Preparation adds steps, and some alloys are simply harder to coat evenly. |
| Sealing | Whether the open pores stay open. Polymer, sol-gel, and conversion seals fill the outer layer. | A second process step with its own qualification. Often the largest single gain available. |
The last row deserves emphasis. If a magnesium part has to last more than days to weeks in a chloride environment, the published literature points the same way again and again: PEO alone is rarely enough, and PEO with a seal usually is.
What we measured
Salt-spray and long immersion tests give the final answer, but they take weeks. For development we need a number within the hour, so we use electrochemical impedance spectroscopy (EIS).
The coated part is exposed to buffered saline (0.9% sodium chloride, pH 7.4) over a small, defined area. We apply a small AC voltage across a range of frequencies and record the impedance. The value at low frequency reflects how well the barrier layer is blocking the solution. Higher is better. The test ranks coatings against each other quickly and without destroying the part. It does not predict service life on its own.
The measurements below are from coatings we grew on a lean magnesium alloy developed for resorbable implants, using an alkaline phosphate electrolyte and pulsed power.
| Condition | Impedance at 1 Hz |
|---|---|
| Uncoated alloy | about 350 Ω·cm² |
| PEO coated, our baseline settings | 23,000 to 74,000 Ω·cm² |
| PEO coated with a polymer seal | 1,600,000 Ω·cm² |
The coating raises impedance about a hundredfold over bare metal, and nominally identical runs spread across a factor of three. That spread is the resolution of the test, and any claimed improvement has to clear it.
Reading the spectra
Figure 3 shows the full spectrum for one part from each row of the table, drawn as Nyquist plots. Each point is one frequency, running from 10 kHz at the left to 0.1 Hz at the right. The horizontal axis is the resistive part of the impedance and the vertical axis is the capacitive part.
A surface that resists corrosion draws an arc, and the width of the arc is the resistance standing between the solution and the metal. Wider is better. Three things are worth reading from the figure.
- The scale. The arc is about 430 Ω·cm² wide for the bare alloy, about 44,000 for the PEO coating, and about 2.2 million for the sealed coating. Each panel is drawn on its own scale because nothing else would fit. At the scale of the middle panel, the whole first panel would sit inside one of its dots.
- Where the arc peaks. The top of the arc moves from 72 Hz on bare metal to 14 Hz with PEO and 0.5 Hz with the seal. A better barrier responds more slowly.
- How the arc ends. On bare metal the last point drops below the axis. That is the signature of metal actively dissolving. The PEO coating shows the start of the same thing: at the lowest frequencies the arc turns back and just reaches the axis, which means solution has already found the metal at the base of some pores. The sealed coating is beginning to turn but stays well above the axis. The seal has slowed the attack by orders of magnitude. It has not stopped it.
That last feature is the one we watch most closely. As a coating starts to fail, the turn-back appears at higher frequencies, well before anything is visible on the part.
If you have a magnesium part to coat
A few things are worth settling early.
- Specify the job, not the thickness. Tell us the environment and how long the part has to last. That decides the electrolyte and whether a seal is needed. Where you need an acceptance test, consider a barrier measurement alongside thickness.
- Name the alloy. AZ31, WE43, and the magnesium-zinc-calcium alloys each behave differently in the bath.
- Allow for growth. The coating grows partly into the metal and partly outward. On our parts, roughly 70% of the coating thickness appeared as added dimension, so a 13 µm coating added about 9 µm per face.
- Plan the contact point. The part needs an electrical connection during coating, and that spot stays bare. Choose where it goes, or tell us which surfaces must be fully covered.
- Expect to seal. For anything beyond short exposure in salt solution, treat the seal as part of the coating from the start.
Further reading
- G. Barati Darband, M. Aliofkhazraei, P. Hamghalam, N. Valizade, “Plasma electrolytic oxidation of magnesium and its alloys: Mechanism, properties and applications,” Journal of Magnesium and Alloys 5 (2017) 74–132.
- T.S.N. Sankara Narayanan, I.S. Park, M.H. Lee, “Strategies to improve the corrosion resistance of microarc oxidation (MAO) coated magnesium alloys for degradable implants: Prospects and challenges,” Progress in Materials Science 60 (2014) 1–71.
- F.C. Walsh, C.T.J. Low, R.J.K. Wood, et al., “Plasma electrolytic oxidation (PEO) for production of anodised coatings on lightweight metal (Al, Mg, Ti) alloys,” Transactions of the IMF 87 (2009) 122–135.